EN 10204 3.1 with every batch · Inspection records before loading sales@hongmingmetal.com WhatsApp +86-177-5175-5597 WeChat 17751755597

Grade comparisons

18/8 and 18/10 Are Sales Names, Not Grade Designations

Neither 18/8 nor 18/10 is a standard grade. Both describe where a heat of 304 sits inside the ASTM A240 chromium and nickel ranges. Write UNS S30400, the product standard and the finish instead.

2026-11-07

Neither 18/8 nor 18/10 appears in ASTM A240. Both are shorthand from the cookware and catering trade for chromium and nickel content, and both sit inside the composition range of one grade: 304.

Where the two numbers come from

The first figure is chromium, the second is nickel, roughly as percentages. ASTM A240 lists 304 as chromium 18.0 to 20.0 and nickel 8.0 to 10.5. A sheet at the lower end of the nickel range is "18/8" and one at the upper end is "18/10", and both are still UNS S30400. A mill does not produce a different alloy to hit the second label. The difference is where that heat falls inside the permitted range.

This is also why the terms cannot serve as an acceptance criterion. There is no test for "18/10", no certificate field for it, and no basis to reject a compliant 304 heat for sitting near the bottom of the permitted nickel range when the enquiry said 18/10.

The confusion with 316

18/10 is sometimes described as "surgical" or "marine" stainless and equated with 316. That is wrong. 316 and 316L are separated from 304 by molybdenum, 2.00 to 3.00 under ASTM A240, not by a higher nickel figure. A nickel reading near 10% on a PMI gun says 304; it says nothing about molybdenum. If chloride service is the reason for asking, work from the 304 vs 316L comparison instead.

What to write instead

Name the grade as 304 / UNS S30400, give the product standard and form (ASTM A240 for sheet and plate, A312 for pipe), state the finish as a designation such as 2B or No.4 rather than "satin", and give the thickness with its tolerance. Add the certificate type. That is a line a mill can produce against and an inspector can check.

For food-contact or catering equipment, the finish and the cleanliness of the surface usually decide more than whether nickel sits at 8 or 10. The surface finish guide covers the designations, and the grade guide explains how the families are named.

If a supplier quotes "18/10 stainless", ask which UNS designation is behind it. The answer tells you whether the quote covers 304 or just a marketing term.

Have a spec you are not sure about? Send the grade, temper and dimensions — we will tell you what the line can actually hold, and what the certificate will say. Request a quote → Related product range: Stainless Steel Sheet & Plate
Tell us the grade, temper and thickness. Quote within 24 hours.
Get a Quote WhatsApp