EN 10204 3.1 with every batch · Inspection records before loading sales@hongmingmetal.com WhatsApp +86-177-5175-5597 WeChat 17751755597

Grades and reference tables

Stainless Steel Composition: What Each Element Does

Ten elements on a certificate, five that decide the outcome. What each one buys, where a heat gets rejected, and the limit that catches it.

2026-11-27

A mill certificate for 304 lists ten elements. Five of them decide what the steel does in service: chromium, nickel, molybdenum, nitrogen and carbon. The other five keep the process honest and occasionally cause a rejection.

Reading them in that order is faster than comparing two data sheets line by line, because each element answers a different question that a buyer actually has.

Chromium sets the floor

Chromium is the element the definition rests on. The 10.5 percent minimum separates stainless from everything else, and above it the tolerance for chloride and oxidizing media rises with the number.

304 carries 18.0 to 20.0 percent. 316L carries 16.0 to 18.0, which looks like a downgrade until molybdenum is counted. 2205 carries 22.0 to 23.0 and adds nitrogen on top.

Nickel buys the structure

Nickel converts the crystal structure from ferritic to austenitic. That is what makes 304 non-magnetic, tough at low temperature, and formable without cracking. 304 holds 8.0 to 10.5 percent, 316L holds 10.0 to 14.0, and 2205 holds only 4.5 to 6.5 because nitrogen and the duplex structure do part of the work.

Nickel is also why a stainless quote moves. It trades on the LME, and many mills recalculate an alloy surcharge monthly against it. Two quotes three weeks apart are often comparing two nickel prices rather than two suppliers.

Molybdenum and nitrogen buy pitting resistance

Molybdenum is what 316L has and 304 does not: 2.00 to 3.00 percent against no specified minimum. It raises the potential at which a pit starts, which is what chloride resistance means in practice.

Nitrogen does similar work at a fraction of the weight, and it is why 2205 reaches its numbers with modest nickel. The combined effect has a shorthand that is worth memorizing:

PREN = Cr + 3.3 Mo + 16 N

304 lands around 18 to 19, 316L around 24 to 26, and 2205 around 35. The step from 304 to 316L is the one that matters for coastal and chlorinated service. The step to 2205 is about strength as much as corrosion.

Carbon decides whether the weld survives

Carbon is the cheapest way to raise strength and the fastest way to ruin a weld. 304 allows 0.07 percent, 316L allows 0.030, and the L is that difference.

Above roughly 0.03 percent, welding takes the metal through 450 to 850 C, where chromium carbides form at the grain boundaries. The chromium tied up in the carbide is no longer available to rebuild the film, so the strip beside the weld becomes the first place to corrode. The L grades stay below the threshold and can be welded without a post-weld anneal.

The elements that cause a rejection

Sulfur is added deliberately for machinability in 303, and is restricted to 0.030 percent in 304 and 316L. Phosphorus sits at 0.045 percent maximum, silicon at 0.75, manganese at 2.00. These are process limits rather than alloying decisions, and a heat that runs over on sulfur or phosphorus is rejected at the mill before it ships.

Element What it does 304 316L 2205
Carbon, max strength, weld decay 0.07 0.030 0.030
Chromium passive film 18.0 to 20.0 16.0 to 18.0 22.0 to 23.0
Nickel austenite, toughness 8.0 to 10.5 10.0 to 14.0 4.5 to 6.5
Molybdenum pitting resistance not specified 2.00 to 3.00 3.0 to 3.5
Nitrogen pitting, strength 0.10 0.10 0.14 to 0.20
Sulfur, max machinability, limited 0.030 0.030 0.020
PREN, typical derived 18 to 19 24 to 26 35

Read a certificate against the ASTM A240 limit for that grade, not against a typical value from a data sheet. A typical value describes a good heat. The limit describes the worst one you have agreed to accept, and the gap between the two is where most arguments about composition start.

Have a spec you are not sure about? Send the grade, temper and dimensions — we will tell you what the line can actually hold, and what the certificate will say. Request a quote → Related product range: Stainless Steel Sheet & Plate
Tell us the grade, temper and thickness. Quote within 24 hours.
Get a Quote WhatsApp